Corona treatment and dyne levels for flexo printing

What corona treatment does to film, recommended dyne levels for water-based, solvent, and UV flexo inks, how to run a dyne test, why treatment decays, and which treatment data belongs on the job record.

Plate area · jobs · customers · AR — one system of record
Flexoworks
  • flexo
  • corona treatment
  • dyne level
  • dyne test
  • surface energy
  • film printing
  • ink adhesion

Corona treatment raises the surface energy of a plastic film so flexo ink can wet it and stick. Surface energy is measured in dynes/cm with test fluids or dyne pens. A common rule of thumb is that the film should read about 10 dynes/cm above the surface tension of the ink. Treatment fades from the moment it is applied, so the reading that matters is the one taken at press.

What corona treatment does

Untreated polyethylene (PE) and polypropylene (PP) have low surface energy, so liquid ink beads up instead of spreading. A corona treater passes the web through a high-voltage discharge between an electrode and a roll. The discharge adds oxygen-bearing groups to the top of the film, which raises its surface energy and gives the ink binder something to bond to. Flame and plasma treating do the same job by other means.

Most film is treated at extrusion and then treated again on press, just before the first print station. That second pass is called bump treating. Pillar Technologies notes it is common for film suppliers to treat to 38 to 40 dynes/cm and expect the printer to bump treat to 42 to 45 dynes/cm for water-based inks.

Substrate Water-based ink Solvent-based ink UV ink
PE 38–44 36–40 38–50
PP 38–44 38–40 40–50
PET 44–52 40–46 42–54
PVC 38–44 36–40 36–50
PS 38–44 35–40 42–48

These are Enercon's flexo and gravure starting ranges in dynes/cm, not acceptance limits. Confirm the target with the ink supplier and the converter's own tests.

Water-based inks need more treatment than solvent inks because water has a higher surface tension than alcohol. Enercon puts water-based flexo inks at 35 to 38 dynes/cm and recommends treating the film to 45 to 48. UV inks run around 50 dynes/cm, so UV jobs sit at the top of the table. The test standard, ASTM D2578, says 35 dynes/cm or higher is generally acceptable for tubular Type 1 PE film for commercial flexo printing, and that wetting tension alone is not a complete measure of ink adhesion.

How to run a dyne test

Enercon describes three methods:

  • Dyne pens. The press-side check. Draw the pen across the web and watch whether the line holds or breaks into beads. Pens also show which side is treated and catch backside treatment. Date them when opened and replace them after about six months.
  • Cotton swab and test fluid. The ASTM D2578 method. If the fluid stays intact for two seconds, the film is at least the level printed on the bottle. Step up until a fluid beads.
  • Drawdown rod. The most accurate. A wire-wound rod pulls three bracketing fluids down a sample at the same film thickness.

Accu Dyne's pen procedure adds the habits that keep results honest: test at least three points across the web (1/4, 1/2, and 3/4), never retest the same spot, keep pens at room temperature, and expect about ±2 dynes/cm precision. Pull the sample as close to the print station as you can. One dyne-testing guide warns that a near-immediate loss of 10 dynes/cm is possible from contact with process rolls, additives blooming to the surface, and transfer inside the wound roll.

Dyne decay and over-treatment

The FTA puts it plainly: all materials suffer dyne decay from the moment they are treated, and the rate changes from roll to roll and supplier to supplier. Slip additives that migrate to the surface speed it up. That is why a roll that passed incoming inspection can fail on press weeks later.

More treatment is not always better. The same dyne-testing guide says raising surface energy by more than 10 to 12 dynes/cm in one pass is often inadvisable, because it can cause pinholing, surface damage, and faster decay. Backside treatment, which happens when air is trapped between the web and the ground roll, can cause blocking and poor heat sealing, according to Enercon's APR presentation. Treaters also make ozone, which is one reason the plate storage note keeps plates away from them.

Rule out treatment before remaking plates

Ink beading, pinholes in solids, poor trapping of one ink over another, and ink lifting on tape all get blamed on plates. Check the dyne level first, then the ink's viscosity and pH, and only then the plate. A plate remake costs the trade shop time and the customer plate area; a dyne pen costs a few seconds. ASTM F2252 covers tape testing of ink adhesion on flexible packaging, with pass criteria agreed between the printer and the buyer. The printing defects note covers the other usual suspects.

What to keep on the job record

Record the film type, supplier, and grade, the treated side, the target dyne level, the reading taken at press and how it was taken, the ink system, and the tape-test result. For a trade shop, film and ink set are part of the print condition the plate curves were built for. If a rerun switches film supplier or ink chemistry, the record shows it is a new print condition, and the dot gain curve may need a fresh check before plates are made.

Common questions

What is corona treatment in printing?

Corona treatment is a high-voltage electrical discharge applied to plastic film before printing. It raises the film's surface energy so ink spreads and bonds instead of beading up. Film is usually treated at extrusion and treated again on press, just before printing, to restore what was lost in storage.

What dyne level is needed for flexo printing?

As a starting point, Enercon lists 38 to 44 dynes/cm for water-based flexo ink on PE and PP, 36 to 40 for solvent-based ink, and 38 to 50 for UV ink. PET needs more, about 44 to 52 for water-based ink. A common rule of thumb is about 10 dynes/cm above the ink's surface tension. Confirm the target with the ink supplier.

How do you test the dyne level of a film?

Apply test fluids or dyne pens of known surface tension to the film. If the fluid holds as a continuous film for about two seconds, the surface is at least that dyne level; if it beads up, the surface is lower. Test at least three points across the web, never retest the same spot, and take the sample as close to the print station as possible.

Does corona treatment wear off?

Yes. Dyne decay starts the moment film is treated and varies by film, additives, storage, and handling. Contact with process rolls and additives blooming to the surface can cut the level quickly. That is why printers check dyne level at press and bump treat on press when the reading is low.